Axsail
SURVEY TEST METHODS · ELECTRICAL AND GAS

Hull potential test: checking a boat's cathodic protection with a reference electrode

UPDATED 17 NOVEMBER 2026 · 1 SOURCES

How to run a hull potential test with a silver/silver chloride reference electrode: setup, protection ranges by hull type and the shore power isolation check.

AT A GLANCE
Hull potential test
MEASURES
The voltage of underwater metals against a silver/silver chloride reference electrode, in millivolts
TOOLS
A reference electrode on at least 20 feet of marine-grade wire, and a multimeter set to DC millivolts
WHEN TO USE
Afloat, when anodes wear too fast or too slowly, when there's corrosion on underwater metals, or when a boat is plugged in at a marina
READ WITH
The hull material, whether the metals are bonded, and the galvanic series

A hull potential test measures how well a boat's anodes protect its underwater metals. A silver/silver chloride reference electrode hangs in the water, a multimeter reads the voltage between it and each metal, and the reading is compared with a protection range for the hull type. Southern Boating's corrosion article gives the method and ranges used below. It also shows whether the boat is isolated from the shore power ground.

Setting up

The test is done afloat, in calm water, with shore power unplugged at the boat, not just switched off, and no equipment running.

  1. Connect the reference electrode, on at least 20 feet of marine-grade wire, to the multimeter's negative terminal. Set the meter to DC volts, or millivolts if it has them.
  2. Connect the positive lead to the metal being measured. On a bonded boat, use a clean point on the bonding system, such as a bolt, bus bar or terminal, cleaned with an abrasive pad if needed.
  3. Lower the electrode about two feet below the surface, clear of the hull.
  4. Read and record, then repeat for each underwater metal.

The article recommends measuring every underwater metal on its own even when the boat is bonded, since a difference between them points to a bonding fault. The propeller and shaft need their own reading, because their path through the oil-filled gearbox is a poor conductor and shaft brushes rarely reach the one ohm the bonding connection should have.

Protection ranges in seawater

Boat Protected range
Fibreglass, common underwater metals other than aluminium -750 to -1,100 mV
Timber hull, metals other than aluminium -550 to -600 mV
Steel hull -850 to -1,100 mV
Aluminium No more negative than -1,100 mV

Southern Boating notes the fibreglass range is more conservative than ABYC's. The rule behind all of them: an anode must drive a metal at least 200 mV more negative than its resting voltage. Resting voltages it gives include silicon bronze at -260 to -290 mV, aluminium alloys -760 to -1,000 mV, and 316 stainless in still water -430 to -550 mV.

Over-protection

Most metals aren't harmed by too much protection. Aluminium is the exception: the alkaline solution that over-protection creates attacks it, which is why its limit is -1,100 mV. On timber boats, the same alkali attacks the wood around bonded fittings. Anodes that hardly wear are as much a warning as anodes that vanish, the article adds: it's a sign they aren't working.

The shore power check

With the readings done, plug in the shore power cord and leave the power off. If any reading moves by more than a few millivolts, the boat isn't isolated from the dock's ground and needs a galvanic isolator, or the one fitted isn't working.

For surveyors

Record the hull type, the water, whether the boat was plugged in, and each metal's reading in millivolts. With Axsail, say "reference cell, bonding bus minus 820, shaft minus 540, cord plugged in moves 40" and the readings land as a table with findings on the shaft and the isolation.

Findings to look for

Each page shows how the defect is found, what decides the grade and example findings written up at A, B and C.

UNDERWATER GEAR

Depleted anodes

When sacrificial anodes need replacing, zinc, aluminium or magnesium for your water, what anodes that aren't wasting mean, what a surveyor checks and three example findings graded A, B and C.

How to find and write it up
ELECTRICAL

Stray current corrosion

How stray current corrosion shows up on a boat, why anodes can't stop it, where it comes from on board and at the marina, how it's tested and three example findings graded A, B and C.

How to find and write it up
ELECTRICAL

No galvanic isolator

How the shore power earth links your boat's underwater metals to every boat on the dock, what a galvanic isolator does, what ABYC A-28 asks for, what one costs and three example findings graded A, B and C.

How to find and write it up
UNDERWATER GEAR

Through-hull bonding

Why surveyors disagree on bonding through-hulls, what Nigel Calder and Don Casey advise, when a fitting should be bonded, what a surveyor checks and three example findings graded A, B and C.

How to find and write it up
HULL AND STRUCTURE

Aluminium hull corrosion

How aluminium boats corrode, where pitting hides, the reference cell readings that show an aluminium hull is protected or overprotected, what a surveyor checks and three example findings graded A, B and C.

How to find and write it up

Frequently asked

What should a hull potential reading be?

Southern Boating's corrosion article gives seawater ranges against a silver/silver chloride electrode: -750 to -1,100 mV for a fibreglass boat with common underwater metals other than aluminium, -550 to -600 mV for a timber hull, and -850 to -1,100 mV for steel. Aluminium shouldn't go beyond -1,100 mV.

How much should anodes shift the reading?

The same article says any metal must be driven at least 200 mV more negative than its resting voltage by the anode to be protected. An unprotected metal reads its own resting voltage from the galvanic series.

Can a boat be over-protected?

Yes. Southern Boating says over-protection creates an alkaline solution around the metals, which attacks aluminium and, on timber hulls, the wood next to bonded fittings, a process called delignification.

How do you tell if a boat needs a galvanic isolator?

After the readings, plug the shore power cord in with the power left off. If readings change by more than a few millivolts, the boat lacks isolation from the shore ground and needs a galvanic isolator, or the one fitted isn't working.

Your full survey report, minutes after the walk-round

Dictate as you inspect. Axsail builds the findings and the report for your signature

Start free

More test methods

All test methods
ELECTRICAL AND GAS

Boat battery test

How to test a boat battery, from Trojan, Crown and Lifeline: rested voltage, hydrometer readings, load tests and a full capacity test, and which to trust.

Read the method
ELECTRICAL AND GAS

LPG gas leak test

How a boat's LPG system is checked for leaks: the test point or bubble detector the Boat Safety Scheme requires, the tightness test and regulator lock-up.

Read the method
ELECTRICAL AND GAS

Thermal imaging

How surveyors use a thermal camera on a boat: hot electrical connections, cooling faults and active thermography for wet core, with its limits.

Read the method
HULL AND STRUCTURE

Percussion test (hammer sounding)

How surveyors sound a fibreglass hull for delamination: which hammer or coin to use, tapping every 2 to 3 inches, and telling a dull thud from a bulkhead.

Read the method
HULL AND STRUCTURE

Ultrasonic thickness testing

Ultrasonic hull thickness testing on steel boats and narrowboats: gauge or A-scan, mill tolerance, wastage limits and the 4 mm insurance rule.

Read the method
HULL AND STRUCTURE

Inclining experiment

What an inclining experiment is for, how it is run under the MCA and Red Ensign codes, the 8 weight movements and when a lightweight check will do.

Read the method

Standards to check against

ABYC E-11

AC and DC Electrical Systems on Boats

What ABYC E-11 covers on a boat's AC and DC systems, the rules surveyors check most often, from the 7 inch battery fuse rule to the reverse polarity indicator, and how to cite E-11 in a finding.

What surveyors check

Report templates

FREE TEMPLATE · WORD

Insurance survey

Free Word template for a recreational boat condition and valuation survey report for insurance: each section explained, with the insurer's requirements and the valuation.