Axsail
SURVEY TEST METHODS · HULL AND STRUCTURE

Ultrasonic thickness testing on a steel boat: taking readings and judging wastage

UPDATED 17 NOVEMBER 2026 · 2 SOURCES

Ultrasonic hull thickness testing on steel boats and narrowboats: gauge or A-scan, mill tolerance, wastage limits and the 4 mm insurance rule.

AT A GLANCE
Ultrasonic thickness testing
MEASURES
Remaining steel plate thickness, from the time a sound pulse takes to cross the plate and echo back
TOOLS
An ultrasonic thickness gauge, or an A-scan flaw detector for hidden corrosion; a pit gauge for local pits
WHEN TO USE
Every steel or aluminium hull out of the water, and insurance surveys that state a minimum thickness
READ WITH
The original plate specification, the plate's mill tolerance, and the insurer's stated minimum

Ultrasonic thickness testing measures how much steel is left in a hull plate by timing a sound pulse through it. On steel boats and narrowboats it's the core of an out of water survey, and often what an insurer's renewal hangs on. The harder part is judging the number: there's no agreed wastage limit for small steel craft, and a low reading isn't always loss. The guidance below is from an IIMS discussion paper and Practical Sailor.

Gauge or A-scan

Instrument What it gives Practical Sailor's view
Basic thickness gauge One number, the largest echo Acceptable for new steel or gross estimates of corrosion
A-scan or C-scan flaw detector All the echo data, as a wave form or a plan view Can find hidden corrosion on the far surface before it weakens the plate
Pit gauge Depth of a single pit Better than ultrasound for pits smaller than the transducer

Practical Sailor notes that corrosion on the far side scatters the sound, so the echo goes weak and broad, which an A-scan shows and a simple gauge misses.

Taking readings

The IIMS paper's points for surveyors:

  • Framing is usually out of reach on a narrowboat, so the plating carries the assessment.
  • Pitting is widespread on boats with basic blacking, and base plating is hard to clean and reach fully at most docks.

Reading the number

Mill tolerance. Steel plate is supplied with a tolerance. Under EN 10029 tolerance class D, 6 mm plate can be 6 mm plus or minus 0.75 mm, so a 5.25 mm reading may be as built, not wastage. Plates can also taper.

What was it built to? The paper says the current narrowboat convention is 10/6/4: 10 mm base, 6 mm sides, 4 mm superstructure. Older boats were built to many other specifications, some all-over 3 mm. Trade association guidance and Dave Gerr's scantling formulae both put the minimum effective thickness at about 3 mm.

Wastage limits. Surveyors split between a minimum thickness and a percentage loss. Class societies use 20% and 25% wastage for ships, and the paper notes surveyors have been challenged legally for not requiring repair above 20%. Applied to a 10 mm base, 20% means repairing any pit over 2 mm. The paper suggests 25% of the minimum design thickness as a more proportionate trigger.

The 4 mm rule. Many insurers ask for at least 4 mm at survey, and their requirements differ. The paper calls the 4 mm figure unhelpful and argues it isn't based on design need.

For surveyors

Take readings on a grid by location so the next survey can compare. Write down the original specification if known, the instrument and mode used, and each reading with its location, and say which standard you judged against, whether the insurer's minimum or a percentage loss. With Axsail, dictate as you go, "base plate, aft third, port side, 8.6, pit 2.1 deep", and the readings come out as a table in the out of water survey report.

Findings to look for

Each page shows how the defect is found, what decides the grade and example findings written up at A, B and C.

HULL AND STRUCTURE

Steel hull wastage

How a surveyor gauges a steel hull with an ultrasonic thickness meter, the 25 percent wastage limit used in US Coast Guard guidance, where steel boats corrode, and three example findings graded A, B and C.

How to find and write it up
UNDERWATER GEAR

Depleted anodes

When sacrificial anodes need replacing, zinc, aluminium or magnesium for your water, what anodes that aren't wasting mean, what a surveyor checks and three example findings graded A, B and C.

How to find and write it up
ENGINE AND FUEL

Fuel tank corrosion

Why aluminium fuel tanks corrode under foam, straps and bilge water, what a surveyor can and can't see, what replacing a tank involves and three example findings graded A, B and C.

How to find and write it up

Frequently asked

What is the minimum steel thickness for a narrowboat?

There's no single industry figure. An IIMS discussion paper notes many insurers ask for 4 mm, while trade and design guidance puts the effective minimum design thickness at about 3 mm. Some surveyors work to a percentage loss instead, typically 20 to 25% of the original plate.

Does a low ultrasonic reading always mean wastage?

No, says the IIMS paper. Steel plate has a mill tolerance: 6 mm plate to EN 10029 tolerance class D can be 6 mm plus or minus 0.75 mm, so a reading of 5.25 mm may be the plate as built.

Is a simple thickness gauge good enough for a steel hull?

Practical Sailor says a basic gauge that gives a single number is only acceptable for new steel or gross estimates of corrosion. An A-scan unit shows all the echo data and can find corrosion on the far side before it has measurably weakened the plate.

Can ultrasound measure pitting?

Practical Sailor says pits are often smaller than the transducer, so ultrasound can misjudge their depth. It recommends a pit gauge, and says any steel boat owner should have one.

Your full survey report, minutes after the walk-round

Dictate as you inspect. Axsail builds the findings and the report for your signature

Start free

More test methods

All test methods
ELECTRICAL AND GAS

Hull potential test

How to run a hull potential test with a silver/silver chloride reference electrode: setup, protection ranges by hull type and the shore power isolation check.

Read the method
HULL AND STRUCTURE

Percussion test (hammer sounding)

How surveyors sound a fibreglass hull for delamination: which hammer or coin to use, tapping every 2 to 3 inches, and telling a dull thud from a bulkhead.

Read the method
HULL AND STRUCTURE

Inclining experiment

What an inclining experiment is for, how it is run under the MCA and Red Ensign codes, the 8 weight movements and when a lightweight check will do.

Read the method
HULL AND STRUCTURE

Underwater hull inspection

Underwater hull inspection by diver or ROV: site and visibility limits, the checklist of hull, running gear and openings, and what the diver's report must show.

Read the method
ENGINES AND MACHINERY

Diesel compression test

How to compression test a marine diesel: the kit, testing through injector or glow plug holes, typical readings and what low cylinders point to.

Read the method
ENGINES AND MACHINERY

Borescope engine inspection

How a borescope engine inspection works on a marine engine: access, piston at bottom centre, which optical tip to use, and how to record each cylinder.

Read the method

Report templates

FREE TEMPLATE · WORD

Out of water survey

A free Word template for an out of water boat survey report: the hull below the waterline, moisture readings, running gear and through-hulls, with example wording and example findings graded A, B and C.

Open template
FREE TEMPLATE · WORD

Insurance survey

Free Word template for a recreational boat condition and valuation survey report for insurance: each section explained, with the insurer's requirements and the valuation.

Open template