Axsail
SURVEY TEST METHODS · HULL AND STRUCTURE

Percussion testing a fibreglass hull: hammer sounding for delamination, filler and wet core

UPDATED 17 NOVEMBER 2026 · 3 SOURCES

How surveyors sound a fibreglass hull for delamination: which hammer or coin to use, tapping every 2 to 3 inches, and telling a dull thud from a bulkhead.

AT A GLANCE
Percussion test (hammer sounding)
MEASURES
Changes in the sound and feel of the laminate that point to delamination, voids, filler or wet core
TOOLS
A firm phenolic hammer, a plastic-handled screwdriver for tight spots, a small smooth tack hammer near fasteners, or a large coin
WHEN TO USE
Every fibreglass hull and deck survey, and over any repair, through-hull or hardware fitting
READ WITH
Moisture meter readings, the boat's construction (solid or cored), and what's on the inside of the hull

Percussion testing, or hammer sounding, is tapping a fibreglass hull and listening. Practical Sailor puts it simply: healthy laminate gives a sharp report, delaminated laminate a dull thud. It finds delamination, voids, filler patches and failing core that a visual check misses, and it costs nothing but time. The method below is from Practical Sailor and surveyor David Pascoe.

Choosing the tool

Tool Where Practical Sailor or Pascoe uses it
Firm phenolic hammer The workhorse for decks and hulls, little risk of harm
Plastic-handled screwdriver Tight corners
Small smooth tack hammer, tapped very lightly Near keel bolts, cleats, winches and other fasteners, where delamination sits just below the surface
Large coin or medallion Pascoe's choice for sounding repairs: he finds plastic on plastic dulls the result and a coin shows soft filler a hammer misses

Practical Sailor warns never to tap hard enough to damage the surface.

How to sound a hull

  1. Calibrate your ear. Tap areas you know are good and any you know have failed, and compare the sound and feel.
  2. Work in a grid. On a cored hull, tap every 2 or 3 inches over the whole surface.
  3. Map every suspect return. The hull will sound different over bulkheads, tanks, changes in thickness, cored and solid areas, and inserts.
  4. Check inside. For each suspect area, look for a bulkhead, tank or bag of sails behind it. If there's nothing there, it's the laminate.

Where to look hardest

  • Around through-hull fittings and near signs of damage or repair, where percussion also finds filler patches.
  • Keel attachments, chainplates, winches and cleats. Practical Sailor says these sit in solid glass and fail one or two layers below the surface, often on the inside, so tap both sides where you can reach.
  • Hull-to-deck and bulkhead joints, where Practical Sailor's hammer test listens for loose bulkheads.
  • Repairs on a storm or accident boat. Pascoe sounds the whole hull with a coin when a repair looks sloppy, looking for delamination or large areas filled with putty.

Limits

Practical Sailor says well-built solid hulls almost never delaminate unless they've been hit or water has got behind the gelcoat. Cored hulls are another matter: the bond between skins and core is mechanical, polyester resin doesn't grip the core well, and core delamination robs the hull of much of its strength. For a closer look at a suspect area, it points to ultrasound, where an A-scan meter can find hidden delamination a simple thickness gauge can't.

For surveyors

Pair sounding with moisture meter readings, and record each suspect area by location and size. With Axsail, say "starboard topsides, aft of the chainplate, dull over 20 by 30 centimetres, nothing behind it inside" and it becomes a finding with the photo, ready for the pre-purchase survey report.

Findings to look for

Each page shows how the defect is found, what decides the grade and example findings written up at A, B and C.

HULL AND STRUCTURE

Wet deck core

How water gets into a cored deck, how a surveyor maps it with a moisture meter and a hammer, which readings to trust, what recoring costs and three example findings graded A, B and C.

How to find and write it up
HULL AND STRUCTURE

Wet transom core

How water gets into a cored transom, how a surveyor finds it with a hammer and a moisture meter, what the sounds and cracks mean, what repair involves and three example findings graded A, B and C.

How to find and write it up
HULL AND STRUCTURE

Grounding damage

What a hard grounding does to a fin keel boat, where the hull splits, what a keel smile means, what a surveyor checks inside and out and three example findings graded A, B and C.

How to find and write it up
HULL AND STRUCTURE

Osmotic blistering

What osmotic blistering is, how a surveyor tells it from paint blisters, which moisture readings matter, what treatment costs per foot and three example findings graded A, B and C.

How to find and write it up
HULL AND STRUCTURE

Loose bulkhead tabbing

Why bulkhead and stringer tabbing lets go, what a failed secondary bond looks like, how a surveyor checks it, what repair involves and three example findings graded A, B and C.

How to find and write it up

Frequently asked

What does a delaminated hull sound like when tapped?

Practical Sailor says healthy laminate gives a sharp report and delaminated laminate a dull thud. The hull will play more than two notes, so map every suspect area and check inside for a bulkhead, tank or stowed gear before calling it delamination.

What hammer should I use to sound a fibreglass hull?

Practical Sailor calls a firm phenolic hammer the workhorse, with a plastic-handled screwdriver for tight corners and a small smooth tack hammer tapped very lightly near fasteners. Surveyor David Pascoe prefers a large coin, saying it shows soft fillers a plastic hammer misses.

How closely should you tap a hull?

Practical Sailor says to tap every 2 or 3 inches over the entire hull on a cored boat, and to be especially suspicious around through-hull fittings and near signs of damage or repair.

Do solid fibreglass hulls delaminate?

Practical Sailor says well-built solid hulls almost never delaminate unless they've had impact damage or water has got past the gelcoat. Cored hulls are far more likely to, because the bond between skins and core is mechanical.

Your full survey report, minutes after the walk-round

Dictate as you inspect. Axsail builds the findings and the report for your signature

Start free

More test methods

All test methods
HULL AND STRUCTURE

Ultrasonic thickness testing

Ultrasonic hull thickness testing on steel boats and narrowboats: gauge or A-scan, mill tolerance, wastage limits and the 4 mm insurance rule.

Read the method
HULL AND STRUCTURE

Inclining experiment

What an inclining experiment is for, how it is run under the MCA and Red Ensign codes, the 8 weight movements and when a lightweight check will do.

Read the method
HULL AND STRUCTURE

Underwater hull inspection

Underwater hull inspection by diver or ROV: site and visibility limits, the checklist of hull, running gear and openings, and what the diver's report must show.

Read the method
ENGINES AND MACHINERY

Diesel compression test

How to compression test a marine diesel: the kit, testing through injector or glow plug holes, typical readings and what low cylinders point to.

Read the method
ENGINES AND MACHINERY

Borescope engine inspection

How a borescope engine inspection works on a marine engine: access, piston at bottom centre, which optical tip to use, and how to record each cylinder.

Read the method
ELECTRICAL AND GAS

Boat battery test

How to test a boat battery, from Trojan, Crown and Lifeline: rested voltage, hydrometer readings, load tests and a full capacity test, and which to trust.

Read the method

Report templates

FREE TEMPLATE · WORD

Pre-purchase survey

Free Word template for a recreational boat or yacht pre-purchase survey report: each section explained, with example wording and findings graded by urgency.

Open template
FREE TEMPLATE · WORD

Out of water survey

A free Word template for an out of water boat survey report: the hull below the waterline, moisture readings, running gear and through-hulls, with example wording and example findings graded A, B and C.

Open template