How to run a dye penetrant test on boat fittings with a red dye kit: cleaning, penetrant dwell, removing the excess, and what the test can and can't find.

AT A GLANCE
Dye penetrant test
MEASURES
Cracks and other flaws open to the surface, shown as red lines or dots on white developer
TOOLS
A solvent-removable visible dye kit: cleaner, red penetrant, developer, lint-free cloths
WHEN TO USE
Chainplates, tangs, swage fittings, stanchion bases, welds and other metal fittings where a crack is suspected
READ WITH
The penetrant's product data sheet for dwell and development times

A dye penetrant test shows cracks that are open to the surface of a metal part. A red penetrant soaks into any crack, the excess is wiped off, and a white developer draws it back out, so a crack shows as a sharp red line. On a boat it's used on chainplates, rigging fittings and welds, where a hairline crack can't be seen with the eye. Practical Sailor's point is that it helps tell scratches from real cracks. The method below is from Magnaflux, which makes penetrant kits.

The solvent-removable method

For work on board, away from a water supply, Magnaflux's Method C, solvent removable, with a visible red dye is the practical choice:

  1. Pre-clean. Remove grease, oil, old residues and, outdoors, every trace of water or ice. Magnaflux recommends a solvent cleaner, which evaporates and leaves the surface dry.
  2. Apply penetrant to the area.
  3. Dwell. 5 to 60 minutes in the process guide; 10 to 30 minutes in the quick start guide. Magnaflux says the product data sheet for the penetrant governs.
  4. Remove the excess. Spray cleaner onto a clean, dry, lint-free cloth, never onto the part, and wipe gently once or twice with a clean area each time. Wiping too hard or too often pulls penetrant out of the cracks.
  5. Apply developer over the area.
  6. Develop. 10 to 60 minutes.
  7. Inspect in good light. A crack shows as red against the white developer.

What it finds and what it misses

Can find Can't find
Cracks, laps and seams open to the surface Flaws below the surface
Fatigue and overload cracks in metal and other non-porous parts Cracks hidden inside fastener holes without taking the fitting apart
Cracks on non-magnetic metals such as stainless and aluminium Anything on very rough or porous surfaces

Practical Sailor notes that cracks often begin inside fastener holes, so the equipment usually has to come apart, though T-ball slots can often be checked in place. It also suggests practising on a bolt bent until a crack just starts, so you know what a real indication looks like.

For surveyors

Say what was tested, which kit and method, the dwell and development times, and what showed, with a photo of the developed surface. With Axsail, say "starboard aft lower chainplate, dye penetrant, red line 6 millimetres at the upper bolt hole" and it's filed on the rig survey report with the image.

Findings to look for

Each page shows how the defect is found, what decides the grade and example findings written up at A, B and C.

RIG

Chainplate crevice corrosion

Why stainless chainplates corrode where they pass through the deck, what a surveyor can see without pulling them, the signs that mean replacement, costs and three example findings graded A, B and C.

How to find and write it up
RIG

Cracked swage terminals

Where standing rigging fails, how a surveyor spots cracked swage terminals and broken strands, the rigging age insurers look for, what re-rigging costs and three example findings graded A, B and C.

How to find and write it up
GAS AND SAFETY

Lifelines and stanchions

Why lifelines fail, why plastic-coated wire hides corrosion, how much load a stanchion base takes, what to check on survey, and three example findings graded A, B and C.

How to find and write it up

Frequently asked

How does a dye penetrant test work?

Magnaflux explains that a penetrant is applied to the part, the excess is removed, and a developer draws penetrant back out of any crack to the surface. A visible red dye shows against the white developer, so a crack appears as a red line.

How long should the penetrant dwell?

Magnaflux's process guide gives 5 to 60 minutes of penetrant dwell and 10 to 60 minutes of development, and says the product data sheet for the penetrant governs. Its quick start guide shows 10 to 30 minutes of dwell.

Can dye penetrant find cracks inside a fitting?

No. Magnaflux says the method detects flaws open to the surface. Practical Sailor adds that cracks often start inside fastener holes, so fittings usually have to come apart to be checked.

How do you remove excess penetrant without washing out the crack?

For the solvent-removable method, Magnaflux says to spray the cleaner onto a clean, dry, lint-free cloth, never directly onto the part, and wipe once or twice with minimal pressure, using a clean area of cloth each time.

Your full survey report, minutes after the walk-round

Dictate as you inspect. Axsail builds the findings and the report for your signature

Start free

More test methods

All test methods
RIG AND DECK

Rig tension gauge

How to use a rig tension gauge on a sailboat, from Loos and Selden's instructions: taking a reading, target tensions and the folding rule method.

Read the method
HULL AND STRUCTURE

Percussion test (hammer sounding)

How surveyors sound a fibreglass hull for delamination: which hammer or coin to use, tapping every 2 to 3 inches, and telling a dull thud from a bulkhead.

Read the method
HULL AND STRUCTURE

Ultrasonic thickness testing

Ultrasonic hull thickness testing on steel boats and narrowboats: gauge or A-scan, mill tolerance, wastage limits and the 4 mm insurance rule.

Read the method
HULL AND STRUCTURE

Inclining experiment

What an inclining experiment is for, how it is run under the MCA and Red Ensign codes, the 8 weight movements and when a lightweight check will do.

Read the method
HULL AND STRUCTURE

Underwater hull inspection

Underwater hull inspection by diver or ROV: site and visibility limits, the checklist of hull, running gear and openings, and what the diver's report must show.

Read the method
ENGINES AND MACHINERY

Diesel compression test

How to compression test a marine diesel: the kit, testing through injector or glow plug holes, typical readings and what low cylinders point to.

Read the method

Report templates

FREE TEMPLATE · WORD

Rig survey

A free Word template for a sailing yacht rig survey report: mast and spars, standing and running rigging, chainplates, furlers and rig age, with example findings graded A, B and C.

Open template